13CrMo4-5
Sources: this site Click: Date: 2015-12-21 2:26:14
Grade : | 13CrMo4-5 |
Number: | 1.7335 |
Classification: | Alloy special steel |
Density: | 7.85 g/cm ³ |
Standard: | EN 10028-2: 2009 Flat products made of steels for pressure purposes. Non-alloy and alloy steels with specified elevated temperature properties | EN 10222-2: 2000 Steel forgings for pressure purposes. Ferritic and martensitic steels with specified elevated temperature properties | EN 10216-2: 2014 Seamless steel tubes for pressure purposes. Technical delivery conditions. Non-alloy and alloy steel tubes with specified elevated temperature properties | EN 10253-2: 2007 Butt-welding pipe fittings. Non alloy and ferritic alloy steels with specific inspection requirements | EN 10273: 2007 Hot rolled weldable steel bars for pressure purposes with specified elevated temperature properties |
|
Chemical composition % of grade 13CrMo4-5 (1.7335): EN 10028-2-2003According EN 10216-2 chemical composition: 0.1 < C < 0.17; 0.4 < Mn < 0.7; |
C | Si | Mn | P | S | Cr | Mo | N | Cu |
0.08 - 0.18 | max 0.35 | 0.4 - 1 | max 0.025 | max 0.01 | 0.7 - 1.15 | 0.4 - 0.6 | max 0.012 | max 0.3 |
Mechanical properties of grade 13CrMo4-5 (1.7335)
Nominal thickness (mm): | to 60 | 60 - 100 | 100 - 150 | 150 - 250 |
|
Rm - Tensile strength (MPa) | 450-600 | 440-590 | 430-580 | 420-570 |
Nominal thickness (mm): | to 16 | 16 - 60 | 60 - 100 | 100 - 150 | 150 - 250 |
|
ReH - Minimum yield strength (MPa) | 290-300 | 290 | 270 | 255 | 245 |
|
KV - Impact energy (J) transverse, | +20° 27 |
|
KV - Impact energy (J) longitud., | +20° 40-44 |
|
A - Min. elongation at fracture (%) | 19-22 |
Equivalent grades of grade 13CrMo4-5 (1.7335)Warning! Only for referenceUSA - | Germany DIN,WNr | Japan JIS | France AFNOR | England BS | Italy UNI | Spain UNE | China GB | Sweden SS | Poland PN | Czechia CSN | Austria ONORM | Russia GOST | Inter ISO |
| | | | | 14CrMo3 | 14CrMo4-5 | 14CrMo4.5 |
| | | | | | | | |