Home » Events » Technical Info » EN Standards
P355N ( 1.0562 )
Sources: this site Click: Date: 2015-12-12 0:4:9
Grade : | P355N | ||||
Number: | 1.0562 | ||||
Classification: | Non-alloy room temperature quality steel | ||||
Standard: |
|
According EN 10216-3:2014: C=<0.2; 0="" 9="<" mn="<1.7;" s="<0.02;" n="<0.02;" ti="<0.04; |
C | Si | Mn | Ni | P | S | Cr | Mo | V | N | Nb | Ti | Al | Cu | - |
max 0.18 | max 0.5 | 1.1 - 1.7 | max 0.5 | max 0.025 | max 0.015 | max 0.3 | max 0.08 | max 0.1 | max 0.012 | max 0.05 | max 0.03 | max 0.02 | max 0.3 | Nb+Ti+V < 0.12 |
Mechanical properties of grade P355N (1.0562)
Nominal thickness (mm): | to 60 | 60 - 100 | 100 - 150 | 150 - 250 |
Rm - Tensile strength (MPa) (+N) | 490-630 | 470-610 | 460-600 | 450-590 |
Nominal thickness (mm): | to 16 | 16 - 40 | 40 - 60 | 60 - 100 | 100 - 150 | 150 - 250 |
ReH - Minimum yield strength (MPa) (+N) | 355 | 345 | 335 | 315 | 305 | 295 |
KV - Impact energy (J) transverse, (+N) | -20° 27-30 | 0° 35-40 | +20° 39-50 |
KV - Impact energy (J) longitud., (+N) | -20° 40-45 | 0° 47-65 | +20° 55-75 |
Nominal thickness (mm): | to 60 | 60 - 250 |
A - Min. elongation at fracture (%) (+N) | 22 | 21 |
Equivalent grades of grade P355N (1.0562)
USA - | Germany DIN,WNr | Japan JIS | France AFNOR | England BS | Italy UNI | Spain UNE | China GB | Sweden SS | Finland SFS | Russia GOST | Inter ISO | ||||||||||||||
|
|
|
|
|
|
|
|
|
|
|
|
Previous: 16Mo3 ( 1.5415 )
Next: P355Q ( 1.8866 )